Causes and measures of welding pores in steel tube
Weld pipe weld porosity affects not only the pipeline denseness, resulting pipeline leakage and corrosion will be induced point seriously reduce the weld strength and toughness. Factors weld porosity are: the flux in the water, dirt, oxide and iron filings, welding ingredients and cover thickness, surface quality steel and steel side plates processing, welding technology and steel molding processes. Related prevention measures: 1. Flux ingredients. CaF2 and SiO2 containing an appropriate amount of welding, the reaction will absorb large amounts of H2, generating a high stability of the HF insoluble in the liquid metal, thereby preventing the formation of hydrogen gas holes. 2. The bulk thickness of the flux is generally 25-45mm, large solder particle size, bulk density hour take the maximum thickness, whereas the minimum value; high current, low welding speed accumulation take the maximum thickness, whereas the minimum value addition, summer or air humidity, flux recove...