Cracking of casing tube
Macroscopic analysis of cracking Casing pipe crack direction for the horizontal, crack propagation along the circumference, the circumference of about 460mm. The flow can flow from the outer wall of the casing along the middle of the crack into the <24415mm casing, indicating that part of the crack has penetrated the casing wall thickness. The main process of casing production is as follows: Furnace refining → continuous casting → ring furnace heating → perforation → rolling → stepping furnace → sizing → sawing → quenching and tempering → straightening → physical and chemical testing → inspection → thread processing → coupling machine tight → water pressure test → Measuring length weighing, marking → packaging storage. Wherein the continuous casting billet is fed into the annular furnace for about 2.5 hours and then perforated at about 1250 °C, followed by continuous rolling at a sizing temperature of 950 ...